Transcript
  • SM490A

    1 1 1 2 2* 3

    1 2 3

    (Flux Cored Arc WeldingFCAW)

    CO2 AWS A5.20 E70T-1 JIS G3106 SM490A

    SM490A

    1.

    Inert-Gases Shield Metal Arc

    Welding

    (Flux-Cored Arc

    Welding, FCAW)

    (weld metal)(heat affected

    zone)

    (reheated zone)

    (primary fusion zone)

    SM490A

  • 9

    mm

    2.

    2.1

    SM490A

    (Niobium)

    SM490A []

    JIS [] JIS G3106 SM490A 16mm

    JIS G3106

    (%) C Mn P S Si Al Nb

    SM490 0.12 1.06 0.02 0.006 0.01 0.032 0.023

    Yield

    Strength (MPa)

    Tensile Strength (MPa)

    Elongation (%)

    JIS G3106 SM490A 325 490-610 17

    Test Result SM490A 457 537 17.3

    JIS

    2.2 FCAW

    (FCAW)

    (over-matching)

    SM490A TM-70C [3]

    1.2mm AWS A5.20

    E70T-1

    (wt%) Fe C Mn P S Si

    E70T-1 Bal. 0.05 1.47 0.017 0.01 0.55

    Yield strength (MPa)

    Tensile strength (MPa)

    Elongation (%)

    E70T-1 549 598 26

    2.3

    (1)

    SASBSC

    SVIQ *= (1)

    (QI V S)

    2.4

    2.4.1

    SiC #240#400#600#800#1000#1500#2000

    0.05m

    5%Nital (5%HNO3+ 98%

    ) OM

    Welding parameters No.

    Welding layer

    Current(A)

    Voltage (V)

    Speed (mm/s)

    Heat input(KJ/mm)

    Total heat input

    (KJ/mm)

    Root 175 25.5 2.33 1.915 Second layer 170 27.5 2.33 2.006

    SA

    Surface 170 29.5 2.33 2.152

    6.073

    Root 165 24.5 2 2.021 Second layer 160 26.5 2 2.12

    SB

    Surface 160 28.5 2 2.28

    6.421

    Root 185 27.5 2.5 2.035 Second layer 180 29.5 2.5 2.124

    SC

    Surface 180 31.5 2.5 2.268

    6.427

  • SEM

    2.4.2 TEM

    3mm 10mm

    200m 70m

    twin-jet (jet polish)

    5%(HClO3) + 20% + 75%

    -15~-10 JEOL JEM 100CXII

    100KV

    2.5

    2.5.1 (tensile test)

    AWS D1.1[4]

    ASTM E8 20mm/min

    2.5.2 (Charpy-notch impact test)

    SEM

    AWS D1.1[4]

    10mm x 7.5mm x 55mm

    2mm ASTM E23

    2.5.3

    SEM

    2.5.4

    AWS D1.1[4]

    40mm x 9mm x 150mm 3-11

    ASTM E190-92

    ()

    ASTM E190-92

  • 2.5.5

    5%nital

    HAZ

    200g 0.5mm

    0.25mm

    2.6 -

    (potentiodynamic polarization curve test)

    (cyclic polarization curve test)

    3.5wt%NaCl ()

    3.

    3.1

    SM490A

    [5](Nb)

    [6] 1200

    (Coarse grain

    zone) (Fine grain zone) (Partially

    transformed zone)(Tempered zone)

    (Reaustenization)

    SM490A

    SM490A

    ( 1200

    )

    [7]

    TEM

    100nm

    SM490A

    50m

  • (grain

    boundary ferrite)(Widmanstatten ferrite)

    (acicular ferrite) (inclusion)

    (Micro-phase)...

    TEM

    5

    1~101

    micro-phase micro-phase

    3.2

    3.2.1

    [8] SM490A

    SM490A

    (MPa) EL

    SM490 537 17.3%

    SA 606 26.47%

    SB 600 25.68%

    SC 599 23.78%

    3.2.2

    (weldability)

    [4]

    (Hv)

    SM490A

    Microphases Microphases

    [6]

    SM490A

    NbNb

    (Ar3)

    Micro-phase

  • SA

    SA

    Gowrisankar[9]

    Dorschu Stout[10]

    Weld Maximum Minimum SM490A170

    180

    190

    200

    210

    220

    230

    240

    250

    HV 0

    .2

    Distance (mm)

    SA SB SC

    Weld Maximum Minimum SM490A

    170

    175

    180

    185

    190

    195

    200

    205

    210

    HV 0

    .2

    Distance (mm)

    SA SB SC

    Weld Maximum Minimum SM490A

    180

    190

    200

    210

    220

    230

    HV 0

    .2

    Distance (mm)

    SA SB SC

    3.2.3

    AWS1.1 4.8.3.3

    1. 1/8inch(3mm)

    2. 1/32inch(1mm) 1/8inch(3mm)

    3/8inch(9.5mm)

    3. (Corner crack)1/4inch(6mm)

    1/8inch(3mm)

    SA SB SC

    SA SB SC

    3.2.4

  • Charpy V-notch

    25C

    ~

    notch

    n*(n

    )

    EDX

    inclusion

    [11]

    DA

    inclusion

    inclusion

    inclusion [10][11]

    SM490

    Nb

    Nb

    SM490A

    [12] EDX (

    ) MnS

    (I)

    SM490A 12.512 0.250791

    HAZ-SA 8.08 0.75896

    HAZ-SB 8.44 0.680468

    HAZ-SC 8.69 0.470208

    W-SA 17.21 0.586228

    W-SB 17.00 1.220092

    W-SC 19.44 0.666107

    SA SB

    SC

  • EDX

    3.3

    3.3.1

    (corrosion potential)

    Tafel (Tafel extrapolation)

    (corrosion current)

    Tafel 50mV

    Tafel

    50mV

    (linear polarization

    method)

    10mV

    SA

    SBSC 2

    order 3 order

    3.5wt%NaCl

    1E-7 1E-6 1E-5 1E-4 1E-3 0.01-1.2

    -1.0

    -0.8

    -0.6

    -0.4

    -0.2

    0.0

    0.2

    0.4

    Pot

    entia

    l (V

    )

    Log I (A/cm2)

    SM490A

    1E-10 1E-9 1E-8 1E-7 1E-6 1E-5 1E-4 1E-3 0.01-1.2

    -1.0

    -0.8

    -0.6

    -0.4

    Pot

    entia

    l (V

    )

    Log I (A/cm2)

    SA SB SC

    mV

    (A/cm2)

    (ohm*cm2)

    BM-SM490 -699 5.578*10-5 6.082*102

    WM-SA -665 5.31 x 10-6 5.876*103

    WM-SB -669 3.38 x 10-8 1.156*106

    WM-SC -652 2.69 x 10-8 1.408*106

    SM490A

    SA SB

    SC

  • 3.3.2

    SM490A 3.5wt%NaCl

    SM490A

    (Positive Pitting hysteresis loop)

    SM490A

    (negative pitting

    hysteresis loop)

    1E-7 1E-6 1E-5 1E-4 1E-3 0.01

    -1.0

    -0.5

    0.0

    0.5

    1.0

    1.5

    Pote

    ntia

    l (V

    )

    Log I (A/cm2)

    SM490A

    1E-7 1E-6 1E-5 1E-4 1E-3-1.5

    -1.0

    -0.5

    0.0

    0.5

    1.0

    Pot

    entia

    l (V

    )

    Log I (A/cm2)

    SA

    1E-7 1E-6 1E-5 1E-4 1E-3-1.5

    -1.0

    -0.5

    0.0

    0.5

    1.0

    Pot

    entia

    l (V

    )

    Log I (A/cm2)

    SB

    1E-8 1E-7 1E-6 1E-5 1E-4 1E-3-1.5

    -1.0

    -0.5

    0.0

    0.5

    1.0

    Pote

    ntia

    l (V

    )

    Log I (A/cm2)

    SC

    BM-SM4

    90A

    SA SB SC

    mV -684 -737 -671 -660

    (A/cm2) 3.312*10-5 3.79*10-6 5.733*10-6 3.88*10-7

    (mV) 148 320 271 204

    (mV) -632 242 - -

  • 4.

    inclusion micorphase

    SM490A

    SM490A

    SM490A

    [1] JIS G3106-2004 Rolled Steels for Welded

    Structure(2004)

    [2] (2008)

    [3] -490/FCAW-G (2008)

    [4] ANSI/AWS D1.1/D1.1M:2002 Structural Welding Code

    - Steel (2002)

    [5]

    P11(1990)

    [6] Najma Shams, Jounal of Materials, 1985, p.21.

    [7] M.N.Waton, P.L.Harrison and R.A. Farrar, Welding and

    Metal Fabrication, 1981, p.101.

    [8] -(1995).

    [9] I. Gowrisankar, A. K. Bhaduri, V. Seetharaman, D. D. N.

    Verma, D. R. G. Achar, Effect of Number of Passes on

    the Structure and Properties of Submerged Arc Welds of

    AISI Type of 316L, Welding JOURNAL, Vol66, 1987,

    p.147-p.154.

    [10] Gladman, Effect of Second-phase Particle on the

    Mechanical Properties of Steel, Iron and Steel

    Interstitute, 1971.

    [11] J.F.Knott, Fundamentals of Fracture Mechanics,

    Butterworth, 1973.

    [12] T.J. Baker and J.A. Charles, Deformation of MnS

    inclusions in steel, J. Iron Steel Inst. 210 (1972),

    p.680p.690.


Top Related